I Have 100 Candles That Started Sweating Before Dispatch — How Do I Decide Whether They Can Be Corrected or Should Be Rejected?

I Have 100 Candles That Started Sweating Before Dispatch — How Do I Decide Whether They Can Be Corrected or Should Be Rejected?

 

Melt containers ₹147.50 for 5 CSI 464 from ₹260.00 Arch Ceramic Burner ₹224.20
100 sweating candles before dispatch
Decide unit by unit what can be saved, and fix the cause before you correct any of them.
★★★☆☆
"Warm comforting fragrance"
M AVerified buyer · Sep 2025
Autumn
★★★★★
"One of the best wax for container Candles. Easy to work with, especially if you are a beginner."
ThenirvaofficialVerified buyer · Nov 2025
Luxury Soy Wax CSI 464 (Flakes Form) For Container Candles
★★★★★
"Love Quality wise fragrance wax loved all the products specially wax melter made easy my life.. thnx i am giving Quality wise 5 stars !!!"
Deepika k.Verified buyer · Mar 2026
Soy Pillar Wax (Specially made for Pillar and Designer Candles)
★★★★★
"Very good"
Radhaa SVerified buyer · Apr 2026
40 Cavity Square Moulds
★★★★★
"Soy pillar wax is really so good"
Jinal PatelVerified buyer · Sep 2025
Soy Pillar Wax (Specially made for Pillar and Designer Candles)
★★★★★
"the quality of luxury soy wax and pillar candle wax is very good, and the packaging is also nice and clean. Do give a try guyss ,ig i have found my candle making supplier! And yes their shipment charges were too higb for me! Other wise the quality is top noch"
Mahak agarwalSep 2024
Soy Pillar Wax (Specially made for Pillar and Designer Candles)
★★★☆☆
"Warm comforting fragrance"
M AVerified buyer · Sep 2025
Autumn
★★★★★
"One of the best wax for container Candles. Easy to work with, especially if you are a beginner."
ThenirvaofficialVerified buyer · Nov 2025
Luxury Soy Wax CSI 464 (Flakes Form) For Container Candles
★★★★★
"Love Quality wise fragrance wax loved all the products specially wax melter made easy my life.. thnx i am giving Quality wise 5 stars !!!"
Deepika k.Verified buyer · Mar 2026
Soy Pillar Wax (Specially made for Pillar and Designer Candles)
★★★★★
"Very good"
Radhaa SVerified buyer · Apr 2026
40 Cavity Square Moulds
★★★★★
"Soy pillar wax is really so good"
Jinal PatelVerified buyer · Sep 2025
Soy Pillar Wax (Specially made for Pillar and Designer Candles)
★★★★★
"the quality of luxury soy wax and pillar candle wax is very good, and the packaging is also nice and clean. Do give a try guyss ,ig i have found my candle making supplier! And yes their shipment charges were too higb for me! Other wise the quality is top noch"
Mahak agarwalSep 2024
Soy Pillar Wax (Specially made for Pillar and Designer Candles)
Reviews collected and published through Judge.me on candlemakingsuppliesindia.store. They are general reviews of the products named on each card, not assessments of the advice set out below. Wording is unedited.
✓ Prices verified 26 September 2026, stock checked per size ✓ MSDS and IFRA documentation on request on WhatsApp ✓ Raw materials only — CSI does not sell finished candles
CSI Diagnostics · Sweating Lot Disposition
A sweating lot is not one decision. Grade every unit A, B or C, burn one of each, read the cause from where the sweating units sit, and give each grade its own option: hold, recheck, rework, melts or reject.
A · B · C
grade every unit before deciding anything about the lot · CSI live pricing, September 2026
Quick answers — read this first
Can the 100 candles be corrected, or should they be rejected? Probably some of each. Don't decide for the lot; grade every unit. A: no oil after a blot check. B: a film or a few droplets on the top only. C: pooling, oil at the sides or base, or separation. Each grade has its own options.

What do I do before touching any of them? Find the root cause. Where the C units sit in the pour order, on the shelf, and in the scent list usually tells you whether the problem is the pour session, storage or the formula. A rework that repeats the cause repeats the sweat.

What are the options per grade? A: hold 7 days lidded, recheck, ship only if still clean. B: blot, lid, hold and recheck; any that mark again become C. C: rework by dilution, salvage as wax melts, or reject. A top-up layer of unscented wax is possible but, in our judgement, the weakest option.

How much is at stake? Worked example (Autumn at 10% in CSI 464, 150 g jars): ₹250.22 of materials per candle, ₹25,021.90 for the lot, before labour, freight, packaging and GST.
The short answer
Stop dispatch: nothing in the lot ships until it is graded and the root cause is known.
Grade every unit: A (0 after blot), B (film or droplets on the top), C (pooling, sides, base, separation); burn one of each side by side to the final third.
Act by grade: A hold and recheck; B blot, hold, recheck; C rework, wax melts or reject, only after the root cause is fixed.
What's at stake: in the worked example, ₹13,762.05 in A, ₹7,506.57 in B and ₹3,753.28 in C of materials; the burn sample uses ₹750.66.
100 sweating candles: grade first, then act by grade Widths to scale: 2.4 px per candle. The 55 / 30 / 15 split is a worked example; your counts replace it. 100 candles one lot A · 55 no oil after blot B · 30 film / few droplets C · 15 pooling, sides, separation Hold 7 days, lids on; recheck day 1, 3, 7. Ship only if still 0. Blot, lid, hold 7 days, recheck. Marks again? Drop it to C. Root cause first. Then rework (3238), wax melts, or reject. Burn sample: one unit from each grade, burned side by side to the final third (method: 3237). Root cause (pour order, shelf, scent, load) before any rework: a remelt that repeats the cause repeats the sweat. Grades use the 0–3 surface score (3235): A = 0 after blotting, B = 1–2 on the top only, C = 3, or oil at sides or base.
The lot drawn as a flow, widths to scale per candle: 100 units graded into A, B and C, and each grade routed to its own action. The split is a worked example. The dashed panel is the two things that happen before any unit is reworked: a burn sample of one per grade, and a root cause.
Straight answer
I have 100 candles that started sweating before dispatch. How do I decide whether they can be corrected or should be rejected?
Don't decide for the lot; decide per unit. Stop dispatch, then grade all 100 under a raking light after a blot check: A shows no oil, B has a film or a few droplets on the top only, C has pooling, oil at the sides or base, or visible separation. Before you correct anything, find the cause, because the pattern of grades usually points to it: C units at the end of the pour order suggest the pour session, C units on one shelf suggest storage heat, C spread evenly suggests the formula itself. Burn one unit of each grade side by side to the final third. Then act by grade. A units are held lidded for 7 days and rechecked; they ship only if they stay clean, the burn sample is normal and the root cause doesn't implicate the whole formula. B units are blotted, lidded and held the same way; any that mark again become C. C units are reworked by dilution, turned into wax melts or rejected, whichever the numbers and your market support. In the worked example each candle holds ₹250.22 of materials, so the lot is ₹25,021.90; the grades tell you how much of that you can still recover.
One line: stop, grade every unit A/B/C, burn one of each, find the cause, then hold A, recheck B and rework, melt or reject C.
Only if grade C becomes melts: Wax Melts Containers Empty are ₹147.50 for 5 (₹29.50 each, flat at every pack size), in heart or square, in stock on 26 September 2026. Capacity isn't stated in the text we captured, so test five before ordering fifty.
Buy 5 containers — ₹147.50

Hold the lot and grade every unit

One hundred candles are not one decision. They are a hundred small ones and a single cause.

The instinct with a sweating lot is to treat it as one thing: ship it, fix it or bin it. But sweating is rarely uniform. Some units are oily, some filmed, many clean, and the difference between them is information. Grading turns a vague problem into counts, and counts into money.

Use the cluster's 0–3 surface score from the cycling-protocol post (0 none, 1 film, 2 droplets, 3 pooling) and add the places oil shouldn't be. Lids off, raking light from a phone torch, every unit numbered in pour order if you recorded it. If you're unsure whether a sheen is oil, press kitchen paper flat on it: a translucent mark is oil (the hub's blot-and-look).

Grading card · one line per unit
Grade on the worst finding · record unit number, pour position, shelf, scent, score and photo
Grade What you see Score Worked-example count
A No oil after a blot check; surface dry 0 55
B A film or a few droplets, on the top surface only 1–2 30
C Pooling; oil at the sides or base through the glass; visible separation or a wet channel 3, or any oil below the top 15

The 55 / 30 / 15 split is a worked example so the ₹ figures have something to multiply; your counts replace it. How to tell oil at the base from wet spots on the glass is covered in the oil-at-the-bottom post; oil around the wick only is 3225's subject. Both change the grade, so check before you count.

Grade in one sitting, under one light
Grade all 100 in one session, with the same torch at the same angle, and ideally with a second person rescoring a random ten without seeing your grades. Scores drift when grading is spread across days or rooms, and a lot graded by two moods is two lots. Photograph every B and C with its number in frame; those photos are your evidence at the recheck.
Mistake: wiping the whole lot and shipping the ones that look fine a day later. What it does: a wiped B unit and a clean A unit look the same on dispatch day and different on your customer's shelf. Fix: grade before you wipe, record the grade on the base, and hold before you judge.

Where the sweating units sit tells you why

Map the grades onto the pour order, the shelf and the scent list. The cause is usually in the pattern.

Root cause comes before rework because every correction option (holding, topping up, remelting, even melts) inherits the cause. The full one-variable checklist is 3233; for a lot, the fastest first pass is to see where the Cs are.

Differential table · pattern of grades in a sweating lot
Ranked most common first as editorial judgement · CSI publishes no failure statistics
# Where the C and B units are Likely cause Rules it in Rules it out
1 Spread evenly through the pour Formula: load near what the wax holds for this oil Load at or near both ceilings; other scents at lower loads dry Grades cluster by position or shelf
2 Mostly the last units poured Pour-session temperature or separation in the pot Pot temperature fell through the session First and last units alike (see 3227)
3 One shelf, a window side, near a heat source Storage heat or hot–cool cycling Same pour, different shelf, different grade Grades mixed on every shelf (see 3228)
4 One scent in a multi-scent lot That oil at that load in that wax Same day, same process, other oils dry Every scent sweats (see 3230)
5 Appeared after cold nights or AC switched off Temperature cycling Onset dates follow the weather log Onset unrelated to temperature

In the worked example the lot is Autumn at 10% of total weight in CSI 464: 15 g of oil and 135 g of wax per candle, which is 11.11% of the wax weight. The page states "Recommended fragrance load 7-11% for candles", and the two-ceilings rule caps it at CSI 464's "Fragrance Load Up to 10%"; read conservatively as % of wax, that ceiling is 9.09% of total. Row 1 is therefore the prime suspect, and it matters for disposition: if the formula is at the edge, even grade A units share the thin margin.

The lot-disposition procedure

Grade, sample, cause, then act. In that order.
1
Stop dispatch and quarantine the lotEvery unit of this pour comes off the shipping shelf, including any already packed. Keep them lidded, together, somewhere at ordinary room temperature away from windows.
2
Grade all 100Blot-check, score and photograph each; write the grade and unit number on the base. Tally A, B and C.
3
Map the gradesPour order, shelf and scent against grade. Read the differential table and write down the most likely cause and what would rule it out.
4
Burn one of each gradeA, B and C units side by side, same trim, same room, in sight, logged to about 1 cm of wax left; the log fields and decision rule are 3237's. If the A unit burns unlike a clean reference, the whole lot is suspect for burn, not just surface.
5
Hold A and B for 7 daysB units blotted, both grades lidded, rechecked on day 1, 3 and 7 (judgement). Any A that marks becomes B; any B that marks again becomes C. Re-tally.
6
Decide per grade, fix the cause, record itChoose from the options table, fix the cause in the next pour, and note on your batch sheet what happened to every unit. If the lot ships in summer, the surviving units go through the summer sign-off sheet first.

The burn sample uses three candles, ₹750.66 of materials in the worked example. It is worth it: a lot you ship on the strength of the surface alone could burn badly, and a lot you reject on the strength of the surface alone might have been sound. Costs exclude labour, freight, packaging and GST.

Options by grade, and the ₹ at stake

Each option has a cost, a risk and a condition. None is free.
Disposition options · worked example
Autumn at 10% in CSI 464 · 150 g Clear Glass Jar with Golden Lid · ₹250.22 of materials per candle · CSI live pricing, 26 September 2026
Grade (count) Materials at stake Option Added cost Condition and risk
A (55) ₹13,762.05 Hold 7 days lidded, recheck, ship if still 0 Time only Only if the cause is not the formula for the whole lot; the margin is thin if row 1 applies
B (30) ₹7,506.57 Blot, lid, hold, recheck Time only Units that mark again drop to C; a clean recheck is not a summer pass
B (30) ₹7,506.57 Top-up: a thin layer of unscented wax ₹156.00 for 10 g each, 300 g from a 500 g bag (₹5.20 a unit) Weakest option (judgement): hides the surface, doesn't change the load below; changes fill weight and headspace; first burn is unscented
C (15) ₹3,753.28 Rework by dilution Fresh wax, extra jars, new wicks: maths in 3238 Only after the cause is fixed and a pilot passes
C (15) ₹3,753.28 Salvage as wax melts Containers: 37 × ₹29.50 = ₹1,091.50 (60 g each, worked example) Melts need their own surface and melt test; you must be able to sell them
C (15) ₹3,753.28 Reject, recover the jars Labour to scrape and wash Oil, wax and wicks lost (₹2,337.28); jars worth ₹1,416.00 recovered if undamaged

A top-up is mostly cosmetic

Pouring a thin layer of unscented CSI 464 over a B unit (at 80–85°C in this jar, whose page states "Safe for hot pour up to 85°C") gives it a fresh, dry top. It doesn't change the oil in the candle below, the hot layer remelts part of the surface it lands on, and the first burn is through unscented wax. It also adds weight: a 150 g candle with a 10 g top-up is 160 g, which matters for your label and for headspace (a gap of roughly 1–1.5 cm below the rim is a common rule of thumb). Net-quantity labelling falls under the Legal Metrology (Packaged Commodities) Rules; check current requirements (not legal advice). In our judgement, use a top-up only on units that stay clean through the hold, and then ask whether you needed it at all.

Wax melts: salvage, not a disguise

Grade C wax, scraped out cold, is still wax and oil. Remelted and poured into melt containers, it becomes a product that is heated in a warmer rather than burned on a wick. Autumn's page gives "9-13% for wax melts", so a 10% wax sits inside the oil page's melt figure; no CSI wax page states a melt ceiling. Fifteen C units hold up to 2,250 g if you recover everything. The containers' capacity isn't stated in the text we captured; at a worked-example 60 g per container that is 37 containers. Melts from a wax that sweated as candles can sweat too, so give them the same day 1, 3 and 7 surface checks and a melt test in a warmer before you list them.

Argued against our own interest: if you don't sell wax melts and have no customers asking for them, don't buy containers to turn 15 bad candles into 37 melts nobody wants. Rejecting the C units, recovering the jars and fixing the cause costs you ₹2,337.28 of oil, wax and wicks and buys nothing more from us. That is often the right answer.

Orders due while the lot is on hold

The hold is a week. Your customers need to hear from you before it ends, not after.

A lot that was meant for dispatch usually has orders against it. Grading and a 7-day hold mean those orders wait, and the temptation is to fill the most urgent ones from the units that look best today. The table is our judgement on how to handle that without shipping a problem.

Order handling during the hold · judgement
Which units may fill which orders, and when
Situation What to send Why
Order due before the 7-day recheck Nothing from this lot; tell the customer the date and why (quality hold) An A unit on day 2 has not yet shown whether it stays clean
Order due after the recheck, A units still at 0 A units, if the cause isn't the formula for the whole lot and the burn sample was normal The only units with a clean record
Cause is the formula (row 1) and it is summer Nothing from this lot until the surviving units pass the summer sign-off The whole lot shares the thin margin
Large or corporate order, one scent Replacement units from a corrected pour, after cure and a surface check A customer buying 50 of one scent will notice two oily ones
Customer asks for "the ones that look fine" No B or C units, wiped or not Wiped units can mark again on their shelf

Replacements take longer than a hold: a pour, a cure (Autumn's page states no cure time in the text we captured; many makers cure soy a week or more before selling, which is common practice) and at least a day 1, 3 and 7 surface check. Build that into the date you give the customer, and keep a disposition log: unit number, grade, recheck results, what happened to it (shipped, reworked, melted, rejected) and the order it filled. The log is what lets you answer a complaint months later.

What not to do with a sweating lot

The most expensive mistakes with a sweating lot often happen in the first hour.
What not to do, or buy: Rework before root cause: remelting all 100 at the same load and process repeats the sweat. Buy fresh oil or wax for the lot before the grading and burn sample are in. Vybar (₹156.00 for 50 g) as a rescue: its page says it "prevents mottling and sweating", but it would have to go in at a remelt, in our judgement it is more commonly associated with paraffin work, and results vary by wax; it's a new formula, not a repair. Heat filled jars to empty them: thermal shock is a common cause of cracked glass. Ship B units wiped because the order is due.

The standard for whether a unit that sweated and recovered is fit to sell belongs to the summer-versus-AC sellability post; this page only decides what to do with the lot you have. In our judgement, don't sell visibly sweating candles without testing, and don't let a deadline turn a hold into a shipment.

Products for disposition and salvage

Four products: the salvage containers, the wax for a pilot or replacements, a burner to melt-test salvaged melts, and the worked example's oil. Chosen on page statements, price and stock on 26 September 2026; CSI has no stability data, so nothing is ranked on performance.

1
container · salvage route for grade C
Wax Melts Containers Empty
Grade C wax that you don't rework can become wax melts: a warmer heats wax without a flame, so a melt doesn't need the burn performance a candle does. The page describes "heat-resistant plastic" containers and "classic clamshells", in heart or square. An honest gap: the text we captured states no cavity count or capacity, so we can't tell you how many melts 15 candles make; ask us on WhatsApp, or weigh a water fill of one before ordering. Melts made from sweating wax can sweat too; they need their own surface check. ₹29.50 a container at every pack size.
Size Price Per unit For the lot
Heart or Square · Pack of 5 ₹147.50 ₹29.50 melt test on a few C units
Heart or Square · Pack of 10 ₹295.00 ₹29.50
Heart or Square · Pack of 50 ₹1,475.00 ₹29.50 most of 15 C units’ wax (see capacity note)
Heart or Square · Pack of 100 ₹2,950.00 ₹29.50 no per-unit saving
Worked example: 37 containers at 60 g each = ₹1,091.50. Buy 5 — ₹147.50
2
wax · for top-ups, a rework pilot or replacement units
Luxury Soy Wax CSI 464 (Flakes Form) For Container Candles
The worked-example lot is CSI 464, so any top-up or rework uses CSI 464. The page states "Fragrance Load Up to 10%" and "Pour Temperature 80°C – 90°C"; in the 150 g jar (hot pour up to 85°C) that means 80–85°C. Argued against our own interest: don't order wax for the lot until the root cause and the burn sample are in. If the C units cluster at the end of the pour, the fix is your pour session, and you may need no wax at all beyond a 500 g bag for a rework pilot. Flat per gram from 1 kg to 10 kg, so the big bag saves nothing.
Size Price Per unit For the lot
500 g ₹260.00 ₹0.52/g top-ups or a rework pilot
1 kg ₹507.40 ₹0.51/g flat per gram up to 10 kg
5 kg ₹2,537.00 ₹0.51/g
10 kg ₹5,074.00 ₹0.51/g replacement production
A 10 g top-up from the 500 g bag is ₹5.20 of wax per unit. Buy 500 g — ₹260.00
3
tool · test a salvaged melt before you sell one
Arch Ceramic Burner
If grade C becomes wax melts, melt-test a few in a warmer before listing them: surface after setting, how the scent comes up, and whether oil gathers in the dish. The page says "place a tealight candle beneath the ceramic bowl" and add "a wax melt". An honest limit: a tealight warmer runs differently from electric warmers your customers may use; one test in one burner is a check, not proof of how melts behave in every warmer. If you won't sell melts, skip it.
Size Price Per unit For the lot
One burner ₹224.20 ₹224.20 melt-test a salvaged melt before selling any
One burner for the melt test. Buy the burner — ₹224.20
4
fragrance · spicy fruity · the worked-example lot
Autumn
The worked-example lot is Autumn at 10% in CSI 464. The page states "Recommended fragrance load 7-11% for candles, 9-13% for wax melts" and describes a "warm oak, amber, and vanilla base"; its FAQ suggests it for gifting "particularly around Diwali, Christmas, and other festive occasions". The two-ceilings rule caps the candle at CSI 464's 10%, and read conservatively as % of wax, that ceiling is 9.09% of total, so this lot is at the edge. For salvage, 10% sits inside the page's 9–13% melt figure, which is the oil page's melt guidance, not a wax page ceiling. Argued against our own interest: Autumn is flat per gram from 50 g to 1 kg (₹5.43), so there is no bulk saving; for replacement units, buy what the replacement pour needs, at the load your root cause points to.
Size Price Per gram 150 g candles at 8%
15 g ₹94.40 ₹6.29 1
50 g ₹271.40 ₹5.43 4
100 g ₹542.80 ₹5.43 8
500 g ₹2,714.00 ₹5.43 41
1 kg ₹5,428.00 ₹5.43 83
A lot candle at 10% is ₹250.22 of materials. Buy 100 g — ₹542.80
Diwali is 8 November 2026, 43 days from 26 September 2026. If the lot was for festive orders, grading and the 7-day hold take about a week; replacement units need a pour, a cure and a check on top. Send us the number of replacements and the load your root cause points to for a quote on CSI 464, Autumn, jars and wicks with a GST invoice and dispatch date.
WhatsApp a Diwali quote
The CSI principle
Grade the lot before you judge it, and find the cause before you fix a single unit.
A, B and C each have their own options; the pattern of grades names the cause. Hold A, recheck B, rework, melt or reject C, and never let a deadline turn a hold into a shipment.
"A sweating lot is a hundred decisions and one cause. Make the one before the hundred."
— CandleMakingSuppliesIndia
Why trust this guide

CandleMakingSuppliesIndia sells the wax, oil, melt containers and burner named here, and does not sell finished candles. This page still tells you not to buy wax or oil for the lot before grading, not to buy melt containers you have no market for, and that rejecting the worst units is often right.

Every price was verified on CSI's live store on 26 September 2026; every size in the pick tables is in stock on that date. Oil, wax, container and burner wording is quoted from the product pages; where a page is silent in the text we captured (the melt containers' capacity and cavity count), we say so.

The grades, the 55 / 30 / 15 split, the 7-day hold, the 10 g top-up and the 60 g melt container are worked examples or editorial judgement; sweating statements are tendencies. CSI publishes no stability or lot data; for lot numbers, ask us. For bulk pricing, GST invoicing, and MSDS and IFRA documentation on request, message us on WhatsApp at +91 7397976926.

Frequently asked questions

What should I do with candles that are sweating before shipping?
Stop dispatch and grade every unit: A no oil after blotting, B a film or droplets on top, C pooling or oil at the sides or base. Burn one of each, find the cause from where the sweating units sit, then hold and recheck A and B and rework, melt or reject C.
Can I wipe the oil off sweating candles and sell them?
Not straight away. A wiped unit can sweat again on your customer's shelf. Blot it, lid it, hold it about 7 days and recheck; only units that stay clean and come from a lot whose cause you understand should ship. In our judgement, don't sell visibly sweating candles without testing.
Can I turn sweating candles into wax melts?
Often, yes: scrape the wax out cold, remelt it and pour into melt containers. Check that the oil page's melt figure covers the load, and give the melts their own surface checks and a melt test in a warmer before selling, because they can sweat too.
Does pouring a layer of plain wax on top stop sweating?
It covers the surface; it doesn't change the oil below. It also adds weight and reduces headspace and gives an unscented first burn. In our judgement it is the weakest option; use it only on units that stayed clean through a hold.
How do I find out why only some of my candles are sweating?
Map each unit's grade against its pour position, shelf and scent. Sweating spread evenly suggests the formula; mostly the last units poured suggests the pour session; one shelf suggests storage heat; one scent suggests that oil at that load.
How much money is at stake in a sweating candle batch?
Multiply the materials per candle by the count in each grade. In our worked example (Autumn at 10% in CSI 464, 150 g jar) that is ₹250.22 a candle and ₹25,021.90 for 100, before labour, freight, packaging and GST; grading shows how much is recoverable.
Before a single sweating candle ships
Grade all 100, burn one of each, find the cause, then act by grade.
A units hold and recheck; B units blot, hold and recheck; C units are reworked, turned into wax melts or rejected once the cause is fixed. In our worked example the lot holds ₹25,021.90 of materials; grading tells you how much of it you can save. Send us your counts and photos if you want a second opinion.
Buy melt containers — ₹147.50 for 5 Send your grade counts on WhatsApp
Editorial standards & sources
About this guide: part of CSI's cluster on sweating, oil pooling and separation (3221–3240). This page owns lot disposition for sweating candles before dispatch: A/B/C grading of every unit, a burn sample of one per grade, root cause from the pattern of grades before any rework, options per grade (hold and recheck, top-up, rework, wax-melt salvage, reject) and the ₹ at stake per option. Dilution maths (3238) and the sellability standard (3223) are linked, not repeated.

Customer reviews: The six reviews at the top of this page are genuine, published Judge.me reviews left by CSI customers on the product pages named on each card — 40 Cavity Square Moulds, Autumn, Luxury Soy Wax CSI 464 (Flakes Form) For Container Candles, Soy Pillar Wax (Specially made for Pillar and Designer Candles). They are general product reviews, not assessments of the diagnostic advice on this page. Names, star ratings, dates and products are as recorded by Judge.me and wording is unedited. "Verified buyer" appears only on reviews Judge.me recorded as verified — M A, Thenirvaofficial, Deepika k., Radhaa S, Jinal Patel. The reviews from Mahak agarwal are published but not recorded as verified, and carry no badge. Reviews below five stars are included as published, not filtered out.

Figures verified 26 September 2026, CSI live pricing: Wax Melts Containers Empty (heart or square) Pack of 5 ₹147.50, 10 ₹295.00, 50 ₹1,475.00, 100 ₹2,950.00 (₹29.50 each); Luxury Soy Wax CSI 464 500 g ₹260.00, 1 kg ₹507.40, 5 kg ₹2,537.00, 10 kg ₹5,074.00; Arch Ceramic Burner ₹224.20; Autumn 15 g ₹94.40 (₹6.29/g), 50 g ₹271.40, 100 g ₹542.80, 500 g ₹2,714.00, 1 kg ₹5,428.00 (all ₹5.43/g from 50 g); Clear Glass Jar with Golden Lid (150 gram) Pack of 10 ₹944.00 (₹94.40 each); Eco Candle Wicks Thin (C1) 10 ₹59.00; Vybar 50 g ₹156.00. All in stock on 26 September 2026. Per gram = price ÷ grams; per container or jar = pack price ÷ units; two decimals.

Non-price figures: load is a percentage of total candle weight (150 g at 10% = 15 g oil + 135 g wax = 11.11% of wax). Page wording quoted: CSI 464 load up to 10%, pour 80–90°C; Autumn 7–11% for candles and 9–13% for wax melts (an oil-page melt figure; no CSI wax page states a melt ceiling); 150 g jar hot pour up to 85°C; melt containers "heat-resistant plastic", capacity not stated in the text we captured. The 55 / 30 / 15 split, the 7-day hold, the 10 g top-up, the 60 g container fill, the grading card and the cause ranking are worked examples or editorial judgement; the headspace figure is a common rule of thumb; Legal Metrology: check current requirements, not legal advice. Costs exclude labour, freight, packaging and GST. Diwali 8 November 2026 is a calendar fact.
Back to blog